Electrical Transport — Iron-Based 2D Conductive Metal-Organic Framework Nanostructure with Enhanced Pseudocapacitance

Measurement evidence

Electrical Transport

Iron-Based 2D Conductive Metal-Organic Framework Nanostructure with Enhanced Pseudocapacitance · Stodolka M., Choi J.Y., Flood J. et al. · ACS Applied Nano Materials · 2022 · 2156-2162

4 measurement groups · 6 results

Reported values remain attached to the sample, method, conditions, extraction quality and source location that produced them.

Four-point-probe electrical conductivity

Cu-HHTP pressed pellet · Pellet

Pressed pellets; same measurement setting as Fe-HHTP.

Temperature
293
Geometry
5 mm diameter circular pressed pellet, four-point probe
Context
pristine Cu-HHTP pellet comparison
Measurement source
main p.5 · Results and Discussion · Figure S13
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
room-temperature electrical conductivity5.57 x 10-3 S cm-10.557 S m-1Text
Exact Reported
main p.5 · Results and Discussion · Figure S13

Four-point-probe electrical conductivity

Fe-HHTP pressed pellet · Pellet

Pressed pellets; Keithley SCS-4200 parameter analyser; room-temperature measurement.

Temperature
293
Geometry
5 mm diameter circular pressed pellet, four-point probe
Context
pristine Fe-HHTP pellet
Measurement source
main p.4 · Results and Discussion · Figure S13
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
room-temperature electrical conductivityMarked as a best value within this paper3.55 x 10-5 S cm-10.00355 S m-1Text
Exact Reported
main p.4 · Results and Discussion · Figure S13

Temperature-dependent four-point-probe conductivity and Arrhenius analysis

Fe-HHTP pressed pellet · Pellet

Conductivity measured from 293 K to 373 K; Arrhenius plot linear fit used for activation energy.

Temperature
293-373
Geometry
pressed pellet
Context
pristine Fe-HHTP pellet
Measurement source
main p.4 · Results and Discussion · Figure 4b; Figure S11
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
Arrhenius activation energyMarked as a best value within this paper0.24 eVText
Exact Reported
main p.4 · Results and Discussion · Figure 4b
conductivity at 293 K~0.027 mS cm-1 at 293 K0.000027 S cm-1Figure Axis
Approximate
SI p.S9 · Structural Characterizations · Figure S11
conductivity at 373 K~0.20 mS cm-1 at 373 K0.0002 S cm-1Figure Axis
Approximate
SI p.S9 · Structural Characterizations · Figure S11

Four-point-probe electrical conductivity

Ni-HHTP pressed pellet · Pellet

Pressed pellets; same measurement setting as Fe-HHTP.

Temperature
293
Geometry
5 mm diameter circular pressed pellet, four-point probe
Context
pristine Ni-HHTP pellet comparison
Measurement source
main p.5 · Results and Discussion · Figure S13
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
room-temperature electrical conductivity1.50 x 10-3 S cm-10.15 S m-1Text
Exact Reported
main p.5 · Results and Discussion · Figure S13