Electrochemical impedance spectroscopy / Nyquist impedance plots
I2-incorporated EuL pressed pellet · Pellet
I2-incorporated EuL pellet measured from 25 to 80 degC under anhydrous conditions; frequency range 1 Hz to 1 MHz; applied ac voltage 300 mV; four-probe electrochemical cell.
| Property | Reported value | Normalised value | Uncertainty | Origin and quality | Source |
|---|---|---|---|---|---|
| Activation energy for conductivityMarked as a best value within this paper | 0.602 eV | — | — | Text Exact Reported | 241 · Electrical properties · Fig. 8b |
| Estimated ln(sigma*T) at 25 degC from Fig. 8a | about -8.3 on the Fig. 8a y-axis | — | visual estimate | Figure Axis Approximate | 242 · Electrical properties · Fig. 8a |
| Estimated ln(sigma*T) at 80 degC from Fig. 8a | about -4.7 on the Fig. 8a y-axis | — | visual estimate | Figure Axis Approximate | 242 · Electrical properties · Fig. 8a |
| I2-incorporated EuL conductivity at 25 degC | 8.27 x 10^-7 S cm^-1 at 25 degC | 0.0000827 S m-1 | — | Text Approximate | 241 · Electrical properties · Fig. 8a |
| I2-incorporated EuL conductivity at 80 degCMarked as a best value within this paper | 2.71 x 10^-5 S cm^-1 at 80 degC | 0.00271 S m-1 | — | Text Approximate | 241 · Electrical properties · Fig. 8a |
| EIS applied ac voltage | 300 mV | 0.3 V | — | Text Exact Reported | 238 · Materials and measurements |
| EIS frequency range | 1 Hz to 1 MHz | — | — | Text Exact Reported | 238 · Materials and measurements |
| Equivalent-circuit fit deviation rule | deviation of R, C, L and Q values must be less than 10% | — | — | Text Exact Reported | 2 · Impedance test |
| Conductivity pellet diameter | 0.8 cm / 8 mm | 8 mm | — | Text Exact Reported | 2 · Impedance test |
| Conductivity pellet thickness | 0.12 cm / 1.2 mm | 1.2 mm | — | Text Exact Reported | 241 · Electrical properties |
| Solid iodine conductivity comparison | 7.69 x 10^-8 S cm^-1 | 0.00000769 S m-1 | — | Text Exact Reported | 241 · Electrical properties |