Electrical Transport — Synthesis and changes of conductivities and thermal stabilities of 4,4′-oxybis [N-(3,4-dihydroxybenzilidene) aniline] chelate polymers

Measurement evidence

Electrical Transport

Synthesis and changes of conductivities and thermal stabilities of 4,4′-oxybis [N-(3,4-dihydroxybenzilidene) aniline] chelate polymers · Kaya I., Yildirim M. · Journal of Inorganic and Organometallic Polymers and Materials · 2008 · 325-333

20 measurement groups · 70 results

Reported values remain attached to the sample, method, conditions, extraction quality and source location that produced them.

Four-point probe conductivity with Keithley 2400 electrometer

3,4-HBA monomer, pristine pressed pellet/solid · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
3,4-HBA conductivity at 0 h iodine exposure1.109 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped 3,4-HBA pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
3,4-HBA conductivity after 120 h iodine exposure67521 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
3,4-HBA conductivity after 144 h iodine exposureMarked as a best value within this paper95272 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
3,4-HBA conductivity after 24 h iodine exposure138.4 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
3,4-HBA conductivity after 48 h iodine exposure1580.8 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
3,4-HBA conductivity after 72 h iodine exposure8471.0 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
3,4-HBA conductivity after 96 h iodine exposure32341 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Cd pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Cd conductivity at 0 h iodine exposure1.4406 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Cd pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Cd conductivity after 120 h iodine exposure3.5677 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cd conductivity after 144 h iodine exposure3.5717 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cd conductivity after 24 h iodine exposure2.045 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cd conductivity after 48 h iodine exposure3.0722 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cd conductivity after 72 h iodine exposure3.367 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cd conductivity after 96 h iodine exposure3.5286 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Co pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Co conductivity at 0 h iodine exposure1.5533 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Co pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Co conductivity after 120 h iodine exposure163.87 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Co conductivity after 144 h iodine exposure244.79 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Co conductivity after 24 h iodine exposure6.2321 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Co conductivity after 48 h iodine exposure29.908 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Co conductivity after 72 h iodine exposure73.667 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Co conductivity after 96 h iodine exposure97.998 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Cr pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Cr conductivity at 0 h iodine exposure14.203 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Cr pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Cr conductivity after 120 h iodine exposure290.16 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cr conductivity after 144 h iodine exposure505.07 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cr conductivity after 24 h iodine exposure20.882 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cr conductivity after 48 h iodine exposure28.112 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cr conductivity after 72 h iodine exposure55.445 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cr conductivity after 96 h iodine exposure106.01 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Cu pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Cu conductivity at 0 h iodine exposure1.8307 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Cu pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Cu conductivity after 120 h iodine exposure13733 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cu conductivity after 144 h iodine exposureMarked as a best value within this paper19057 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cu conductivity after 24 h iodine exposure13.076 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cu conductivity after 48 h iodine exposure53.299 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cu conductivity after 72 h iodine exposure232.54 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Cu conductivity after 96 h iodine exposure1782.4 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Mn pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Mn conductivity at 0 h iodine exposure1.4703 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Mn pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Mn conductivity after 120 h iodine exposure11803 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Mn conductivity after 144 h iodine exposureMarked as a best value within this paper18001 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Mn conductivity after 24 h iodine exposure21.07 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Mn conductivity after 48 h iodine exposure187.12 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Mn conductivity after 72 h iodine exposure1030.4 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Mn conductivity after 96 h iodine exposure5910.2 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Ni pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Ni conductivity at 0 h iodine exposure1.5621 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Ni pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Ni conductivity after 120 h iodine exposure1528.5 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Ni conductivity after 144 h iodine exposure4369.1 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Ni conductivity after 24 h iodine exposure5.6112 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Ni conductivity after 48 h iodine exposure14.719 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Ni conductivity after 72 h iodine exposure67.217 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Ni conductivity after 96 h iodine exposure404.71 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Pb pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Pb conductivity at 0 h iodine exposure1.4403 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Pb pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Pb conductivity after 120 h iodine exposure18.969 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Pb conductivity after 144 h iodine exposure20.411 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Pb conductivity after 24 h iodine exposure3.126 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Pb conductivity after 48 h iodine exposure4.7125 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Pb conductivity after 72 h iodine exposure11.147 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Pb conductivity after 96 h iodine exposure15.553 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Zn pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Zn conductivity at 0 h iodine exposure1.8603 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Zn pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Zn conductivity after 120 h iodine exposure17.168 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zn conductivity after 144 h iodine exposure21.309 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zn conductivity after 24 h iodine exposure2.6502 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zn conductivity after 48 h iodine exposure3.3121 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zn conductivity after 72 h iodine exposure4.3905 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zn conductivity after 96 h iodine exposure8.1622 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer

P-3,4-HBA-Zr pristine coordination-polymer solid/pellet · Pellet

Pressed pellet; doping time 0 h; 25 °C table condition; atmospheric pressure/room temperature handling.

Temperature
298.15
Atmosphere
atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
pristine/control value before iodine vapour exposure
Measurement source
4 · Section 2.5 Electrical Properties
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Zr conductivity at 0 h iodine exposure13.701 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2

Four-point probe conductivity with Keithley 2400 electrometer after iodine-vapour doping

I2-doped P-3,4-HBA-Zr pressed pellet time series · Pellet

Pressed pellet exposed to iodine vapour at atmospheric pressure and room temperature; conductivity tabulated at 24, 48, 72, 96, 120 and 144 h; table caption gives 25 °C.

Temperature
298.15
Atmosphere
iodine vapour at atmospheric pressure
Geometry
pressed pellet; four-point probe
Context
iodine-doped sample series
Measurement source
4,7 · Section 2.5 and Table 2 · Table 2; Figs. 5-6
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
P-3,4-HBA-Zr conductivity after 120 h iodine exposure45.713 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zr conductivity after 144 h iodine exposure50.002 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zr conductivity after 24 h iodine exposure16.198 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zr conductivity after 48 h iodine exposure20.104 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zr conductivity after 72 h iodine exposure31.54 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2
P-3,4-HBA-Zr conductivity after 96 h iodine exposure39.017 x 10^-10 S cm^-1Table
Exact Reported
7 · Table 2 · Table 2