Route 1: Drop Cast

3 · 2.5. Modified electrode preparation

Solventsethanol/water 4:1 for diluted Nafion
AdditivesNafion, 0.05%
Atmosphereopen air drying
Time2 h material drying; 0.75 h Nafion drying
Substrate orientationglassy carbon electrode
Work-upprepared in the same way as AgMOF/GCE after material dispersion
Activationair dried
Show 2 structured reagent records
RoleReagentAmount / concentrationSource
OtherAg nanosphere1 mg/ml used for comparison3 · 2.5. Modified electrode preparation
AdditiveNafion solution10 uL · 0.05%3 · 2.5. Modified electrode preparation
Partial recipeSource: Main

Route 2: Other

3 · 2.3. Synthesis of AgMOF-derived Ag nanosphere

Metal precursorsas-synthesised dry AgMOF
Linker precursors2-methylimidazole / Hmim, 0.492 g
Solventsdistilled water; ethanol wash
AdditivesHmim ligand-exchange agent
AtmosphereAr during calcination
Temperatureroom temperature ligand exchange; 700 C calcination
Time0.167 h ligand exchange; 6 h drying; 8 h calcination
Oxidant / reductantHmim ligand exchange/reduction environment; authors describe Ag+ reduction to metallic Ag during transformation
Work-upwashed three times with DI water, followed by ethanol; dried in a hot air oven for 6 h
Activationcalcined 8 h at 700 C in Ar
Show 3 structured reagent records
RoleReagentAmount / concentrationSource
OtherAgMOF solution2.0 mmol in 120 ml distilled water3 · 2.3. Synthesis of AgMOF-derived Ag nanosphere
LinkerHmim solution0.492 gm Hmim in 120 ml3 · 2.3. Synthesis of AgMOF-derived Ag nanosphere
Solventdistilled water120 ml + 120 ml3 · 2.3. Synthesis of AgMOF-derived Ag nanosphere
Complete recipeSource: Main

Route 3: Drop Cast

3 · 2.5. Modified electrode preparation

Solventsethanol/water 4:1 for diluted Nafion
AdditivesNafion, 0.05%
Atmosphereopen air drying
Time2 h material drying; 0.75 h Nafion drying
Substrate orientationglassy carbon electrode
Work-upsonicated material solution 20 min before casting
Activationair dried
Show 2 structured reagent records
RoleReagentAmount / concentrationSource
OtherAgMOF10 uL cast · 1 mg/ml3 · 2.5. Modified electrode preparation
AdditiveNafion solution10 uL · 0.05%3 · 2.5. Modified electrode preparation
Complete recipeSource: Main

Route 4: Solvothermal

3 · 2.2. Synthesis of AgMOF

Metal precursorsAgNO3, 1.435 g
Linker precursorsH2BDC / terephthalic acid, 0.475 g
SolventsDMF, 40 mL
Temperature120
Time20
Work-upcentrifuged 15 min at 6000 rpm; washed thoroughly with DI water then ethanol
Activationdried at 50 C overnight
Show 3 structured reagent records
RoleReagentAmount / concentrationSource
LinkerH2BDC0.475 gm3 · 2.2. Synthesis of AgMOF
SolventDMF40 ml3 · 2.2. Synthesis of AgMOF
Metal SourceAgNO31.435 gm3 · 2.2. Synthesis of AgMOF