Other — Synthesis and characterization of a novel kind soluble, conjugated, and fluorescent chelate polymer containing fluorene ring in the backbone: Optical, electrical, and electrochemical properties

Measurement evidence

Other

Synthesis and characterization of a novel kind soluble, conjugated, and fluorescent chelate polymer containing fluorene ring in the backbone: Optical, electrical, and electrochemical properties · Yildirim M., Kaya I. · Synthetic Metals · 2011 · 13-22

4 measurement groups · 10 results

Reported values remain attached to the sample, method, conditions, extraction quality and source location that produced them.

Differential scanning calorimetry (DSC) using Perkin Elmer Pyris Sapphire DSC

poly(3,4-HBA-Cr-FDA) bulk chelate polymer · Powder

25-420 deg C in N2 at 20 deg C/min.

Atmosphere
N2
Context
pristine polymer
Measurement source
16,19 · 2.3. Characterization techniques; 3.2. Differential scanning calorimetry (DSC) · Fig. 4
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
polymer specific heat change during glass transition0.645 J/g KText
Exact Reported
19 · 3.2. Differential scanning calorimetry (DSC) · Fig. 4
polymer glass transition temperature355 deg CText
Exact Reported
19 · 3.2. Differential scanning calorimetry (DSC) · Fig. 4
polymer DSC hydrate-water removal peak122.71 deg CText
Exact Reported
18-19 · 3.2. Differential scanning calorimetry (DSC) · Fig. 4

ICP-AES using Varian Liberty II Series AX

MC-2 Cr-coordinated dialdehyde · Powder

MC-2 kept at 150 deg C for 3 h before measurement; 0.75 g L^-1 MC-2 solution used.

Context
MC-2 model compound
Measurement source
16-17 · 2.3. Characterization techniques; 3.1. Solubility and structures
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
MC-2 chromium content15.89%Text
Exact Reported
17 · 3.1. Solubility and structures
MC-2 theoretical chromium content16.05%Text
Exact Reported
17 · 3.1. Solubility and structures

Size exclusion chromatography (SEC) using Shimadzu system

poly(3,4-HBA-Cr-FDA) bulk chelate polymer · Powder

SGX column; DMF eluent at 0.4 mL/min; polystyrene standards; RID and UV detectors at 25 deg C.

Temperature
298
Context
pristine polymer
Measurement source
16,18 · 2.3. Characterization techniques; 3.1. Solubility and structures
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
polymer SEC Mn by UV detector42,810 g mol^-1Text
Exact Reported
18 · 3.1. Solubility and structures
polymer SEC Mw by UV detector43,480 g mol^-1Text
Exact Reported
18 · 3.1. Solubility and structures
polymer SEC PDI by UV detector1.016Text
Exact Reported
18 · 3.1. Solubility and structures
polymer repeated unitsapproximately 65-68 repeated units65-68Text
Range
18 · 3.1. Solubility and structures

TGA using Perkin Elmer Diamond Thermal Analysis

MC-2 Cr-coordinated dialdehyde · Powder

20-1000 deg C in N2 at 10 deg C/min to determine hydrate/absorbed water.

Atmosphere
N2
Context
MC-2 model compound
Measurement source
16-17 · 2.3. Characterization techniques; 3.1. Solubility and structures
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
MC-2 absorbed/hydrate water removalapproximately 26% between 20 and 150 deg CText
Approximate
17 · 3.1. Solubility and structures