Complete recipeSource: Main
Route 1: Drop Cast
p003 · Fabrication of the Modified GCE
Metal precursorsNi/Mn-MOF powder already synthesised
Linker precursorsTPA in Ni/Mn-MOF component
SolventsDMF suspension; ethanol/water cleaning solution; deionised-water rinse
Additivesalumina powder for polishing
Atmosphereambient air, not explicitly stated
Temperatureroom temperature
Substrate orientationglassy carbon electrode surface
Work-upGCE polished with alumina, cleaned in ethanol/water, coated with 10 uL suspension, dried at room temperature and rinsed with deionised water.
Activation15 consecutive CV cycles from 0 to 0.5 V at 0.02 V/s in 0.1 M NaOH.
Scalability contextElectrode-scale drop-cast coating.
Show 4 structured reagent records
| Role | Reagent | Amount / concentration | Source |
|---|---|---|---|
| Other | Ni/Mn-MOF powder | 0.5 mg · 1 mg mL-1 in DMF | p003 · Fabrication of the Modified GCE |
| Solvent | DMF | 0.5 mL | p003 · Fabrication of the Modified GCE |
| Electrolyte | NaOH | 0.1 M | p003 · Fabrication of the Modified GCE |
| Additive | alumina powder | Not specified | p003 · Fabrication of the Modified GCE |