Porosity — A 2D copper-imidazolate framework without thermal treatment as an efficient ORR electrocatalyst for Zn-air batteries

Measurement evidence

Porosity

A 2D copper-imidazolate framework without thermal treatment as an efficient ORR electrocatalyst for Zn-air batteries · Franco A., Salatti-Dorado J.I., Garcia-Caballero V. et al. · Journal of Materials Chemistry A · 2022 · 24590-24597

1 measurement group · 6 results

Reported values remain attached to the sample, method, conditions, extraction quality and source location that produced them.

N2 adsorption-desorption at 77 K; BET, t-plot and BJH analysis

as-synthesised 2DCIF nanosheet powder · Nanosheet

Powder evacuated at 150 C for 16 h before measurement

Temperature
77
Atmosphere
N2
Geometry
powder
Context
pristine 2DCIF nanosheets
Measurement source
13 · III.6 N2 physisorption · Fig. S14; Table S3
PropertyReported valueNormalised valueUncertaintyOrigin and qualitySource
BJH average pore size29 nmText
Rounded Reported
24593 · Results and discussion · Fig. S14
external surface area by t-plot18.4 m2 g-1Text
Exact Reported
24593 · Results and discussion · Table S3
BET specific surface area34.5 ± 0.5 m2 g-1± 0.5 m2 g-1SI Table
Exact Reported
13 · III.6 N2 physisorption · Table S3
total pore volume0.18 cm3 g-1Text
Rounded Reported
24593 · Results and discussion · Fig. 2C; Table S3
mesopore volume0.177 cm3 g-1SI Table
Exact Reported
13 · III.6 N2 physisorption · Table S3
micropore volume0.007 cm3 g-1SI Table
Exact Reported
13 · III.6 N2 physisorption · Table S3