Temperature-dependent I-V and conductivity measurement using Keithley 2602B source meter, two-probe method
Cu3(HHTP)(THQ) powder pellet · Pellet
Powder pellet measured in Ar-filled glove box to avoid humidity and interfering gases; Pt electrodes; temperature-dependent I-V curves.
| Property | Reported value | Normalised value | Uncertainty | Origin and quality | Source |
|---|---|---|---|---|---|
| Thermal activation energyMarked as a best value within this paper | 0.30 eV | — | — | Text Rounded Reported | 174 · Results and discussion · Figure 3c |
| Conductivity in air at 35% relative humidity | ca. 5 x 10^-6 S cm^-1 | — | — | Text Approximate | 174 · Results and discussion · Figure 3b,c |
| Room-temperature semiconductivity in ArMarked as a best value within this paper | approximately 2.53 x 10^-5 S cm^-1 | — | — | Text Approximate | 174 · Results and discussion · Figure 3b,c |
| Cu3(HHTP)2 comparator conductivity | ca. 10^-3 S cm^-1 | — | — | Text Approximate | 174 · Results and discussion |
| Cu3(THQ)2 comparator conductivity | ca. 10^-8 S cm^-1 | — | — | Text Approximate | 174 · Results and discussion |
| I-V contact behaviour | linear and zero drift temperature-dependent I-V curves; good ohmic contact | — | — | Qualitative Qualitative | 174 · Results and discussion · Figure 3b |